Fracture toughness of carbides in tool steels evaluated by nanoindentation J. Caro a , D. Casellas a , S. Molas a , J. M. Prado a , I. Valls b a  CTM Centre Tecnològic b  ROVALMA S.A.
INTRODUCTION Ultra high strength steels AHSS (tensile strength> 700 MPa) are increasingly used in automotive industry due to: ,[object Object],[object Object],[object Object],INTRODUCTION
INTRODUCTION INTRODUCTION Premature  fractures < 2000—5000 pieces ,[object Object],Forming of AHSS Accelerated wear and early fractures of forming tools (dies and punches)
INTRODUCTION Cold work tool steels for forming AHSS must be: ,[object Object],[object Object],[object Object],[object Object],[object Object],[object Object],[object Object],[object Object],[object Object],[object Object],Hardness-toughness relationship in tool steels must be optimised INTRODUCTION Wear has traditionally been overcome by increasing hardness, which inevitably leads to a decrease in toughness high wear resistant     high hardness high fracture resistant     high toughness
INTRODUCTION In order to develop high performance tool steels is necessary a detailed knowledge of the relationship between the hardness and fracture toughness of carbides and the macroscopic wear and fracture resistance of the bulk material The micrometric size of primary carbides to be analyzed forces the use of  nanoindentation  techniques  Hardness and Young modulus :  determined by confined indentation on carbides Fracture toughness :  determined by the generation of cracks at the corner of the indentation This work has been recently published in  D. Casellas et al., Acta Materialia  55  (2007) 4277 INTRODUCTION
In brittle materials fracture toughness (K C ) can be determined by the  Indentation Microfracture Method (IM) Types of fracture generated by sharp indenters Halfpenny or radial cracks Connected underneath the hardness impression. The most common crack configuration for brittle materials Palmqvist cracks Developed at low indentation loads or in high-toughness materials (i.e. hard metals or zirconia ceramics) Berkovich  cracks FRACTURE TOUGHNESS FRACTURE TOUGHNESS
Common expression used for K C  determination (depending on indenter geometry and crack morphology): Anstis. :  Limited to radial cracks. Applied to the symmetric indenters (i.e. Vickers) P  indentation load,  c  crack length A = 0.016 and n =0.5 Laugier :  Used for Palmqvist cracks x V  = 0.015 Niihara  :  Used for Palmqvist cracks a : half-diagonal of the impression c = a + l    = 0.0089 (for WC-Co) [1] [2] [3] FRACTURE TOUGHNESS FRACTURE TOUGHNESS
FRACTURE TOUGHNESS FRACTURE TOUGHNESS Berkovich  indenters are generally used in small-scale determination of K C . The most commonly used expression is Anstis equation. However, the  nonsymmetrical nature of  Berkovich  indenters does not permit the radial cracks to be joined beneath the hardness impression  The application of Anstis equation in this case is doubtful Dukino and Swain determined that good K c  values using  Berkovich  indenters are obtained using  Laugier   expression with a little modification (x V  = 0.016)
In this work, K C  of micrometric primary carbides (10-20   m) in tool steels is determined using  Berkovich  indenters at low indentation loads (200-500 mN). It is expected to generate Palmqvist-type cracks (equations 2-3 are expected to give better results than equation 1). It is necessary to generate small cracks (shorten than 5-10   m) within the carbide. At this crack extension application of equations (1)-(3) could give rise to considerable differences in the calculated K C  value. FRACTURE TOUGHNESS FRACTURE TOUGHNESS 9   m
Values of K C  evaluated with expressions (1)-(3) for different primary carbides in different tool steels FRACTURE TOUGHNESS FRACTURE TOUGHNESS
K C  values calculated by the expressions (1)-(3) at P=200 mN and a=2.8  m corresponding to the M 6 C carbides of 1.3202 steel. At short crack lengths Laugier’s expression (3) gives the highest values of K C , 2.4 times larger than Anstis’s expression (1) FRACTURE TOUGHNESS FRACTURE TOUGHNESS
As postulated previously, Laugier’s expression seems to be more appropriate for nanoindentation tests using  Berkovich  indenters. This expression has been successfully proved in a wide range of ceramic materials using  Berkovich  indenters. However, the differences between the results obtained with different expressions should be assessed.  Consequently, the IM method was applied to a material whose K C  is well known using low loads. The results were compared with the K C  values obtained with macroscopic methods based on the propagation and fracture of large cracks reported in the literature. Chosen material    Silicon single crystal Si (100) FRACTURE TOUGHNESS FRACTURE TOUGHNESS
Nanoindentation on Si(100) plane at 200 mN Niihara (2) and Laugier (3) (using x V  = 0.016) expressions give values of K C within the range of the values of Si reported with large crack testing methods FRACTURE TOUGHNESS FRACTURE TOUGHNESS large crack testing methods
Niihara et al. set the applicability of equation (2) within the range 0.4<a/l<1 In our case, almost all the data for the analyzed carbides lie outside this range FRACTURE TOUGHNESS FRACTURE TOUGHNESS
CONCLUSION: All these comments allow us to point out that the evaluation of K C  by nanoindentation using  Berkovich  indenters should be conducted using Laugier expression (with x V  = 0.016): This assertion is specially relevant at low applied loads, when cracks are shorten than 10   m, which usually occurs in nanoindentation of small particles such as in primary carbides of commercial cold work tool steels FRACTURE TOUGHNESS FRACTURE TOUGHNESS
RESULTS ,[object Object],[object Object],[object Object],Analyzed tool steels RESULTS
RESULTS RESULTS Crystal structure was determined by XRD Samples were extracted with the same orientation, parallel to the rolling direction
RESULTS RESULTS ,[object Object],[object Object],[object Object],[object Object],[object Object],Scattering in H, E, K C  values can be due to: Confocal laser microscopy image 0 4.5   m 80   m 60   m
RESULTS RESULTS catastrophic carbide fracture 20   m 20   m catastrophic carbide fracture
RESULTS Hardness and Young modulus of primary carbides RESULTS ,[object Object],[object Object],[object Object],[object Object]
RESULTS RESULTS 1.3202 Steel M 6 C M 6 C MC 7   m 10   m 10   m
RESULTS RESULTS MC-II Steel B 15   m MC-I Steel A 9   m 8   m MC-III Steel B
RESULTS Fracture anisotropy in M 7 C 3  carbides in 1.2379
RESULTS Primary carbides in 1.2379 are  elongated as a consequence of forging steps during fabrication Cracks emanating from the indenter corners propagate preferentially in the direction parallel to the larger edge. XRD study reveal that M 7 C 3  carbides are strongly textured. The observed fracture anisotropy is independent of the tip-carbide orientation and can be attributed to crystallographic anisotropy crystallographic directions  ,[object Object],[object Object],[object Object],Fracture anisotropy in M 7 C 3  carbides in 1.2379
RESULTS RESULTS Arrows for M 7 C 3  in 1.2379 steel indicate that K C  may be even lower Hardness and fracture toughness of different carbides Hard and tough carbides Potential candidates for incorporating in tool steels aimed at optimizing the relationship between wear and fracture resistance
RESULTS RESULTS Toughness (K C ) vs. composition of MC carbides V-rich carbides exhibit high values of K C
RESULTS RESULTS ,[object Object],[object Object],[object Object],[object Object],[object Object],[object Object],[object Object]

Contenu connexe

Tendances

Report on Hardness test
Report on Hardness testReport on Hardness test
Report on Hardness testMarwan Shehata
 
Presentation For Fracture Mechanics
Presentation For Fracture MechanicsPresentation For Fracture Mechanics
Presentation For Fracture Mechanicsaswaghch
 
micro vicker hardness test
micro vicker hardness testmicro vicker hardness test
micro vicker hardness testAbdul Rahman
 
Material Hardness Testers
Material Hardness TestersMaterial Hardness Testers
Material Hardness TestersBilal
 
Fracture Toughness I by Carl Ziegler
Fracture Toughness I by Carl ZieglerFracture Toughness I by Carl Ziegler
Fracture Toughness I by Carl ZieglerSMT_Materials
 
A fracture mechanics based method for prediction of
A fracture mechanics based method for prediction ofA fracture mechanics based method for prediction of
A fracture mechanics based method for prediction ofSAJITH GEORGE
 
IMPACT TEST REPORT ...
IMPACT TEST REPORT                                                           ...IMPACT TEST REPORT                                                           ...
IMPACT TEST REPORT ...musadoto
 
Compression test verification_for_a_wood
Compression test verification_for_a_woodCompression test verification_for_a_wood
Compression test verification_for_a_woodSumitThakur755213
 
Rockwell hardnes testing
Rockwell hardnes testingRockwell hardnes testing
Rockwell hardnes testingUsman
 
Fracture toughness measurement testing
Fracture toughness measurement testingFracture toughness measurement testing
Fracture toughness measurement testingkhileshkrbhandari
 
fracture mechanics presentation
fracture mechanics presentationfracture mechanics presentation
fracture mechanics presentationM Shahid Khan
 

Tendances (20)

Report on Hardness test
Report on Hardness testReport on Hardness test
Report on Hardness test
 
Presentation For Fracture Mechanics
Presentation For Fracture MechanicsPresentation For Fracture Mechanics
Presentation For Fracture Mechanics
 
micro vicker hardness test
micro vicker hardness testmicro vicker hardness test
micro vicker hardness test
 
Material Hardness Testers
Material Hardness TestersMaterial Hardness Testers
Material Hardness Testers
 
Necking
NeckingNecking
Necking
 
Fracture Toughness I by Carl Ziegler
Fracture Toughness I by Carl ZieglerFracture Toughness I by Carl Ziegler
Fracture Toughness I by Carl Ziegler
 
A fracture mechanics based method for prediction of
A fracture mechanics based method for prediction ofA fracture mechanics based method for prediction of
A fracture mechanics based method for prediction of
 
Hardness test en
Hardness test enHardness test en
Hardness test en
 
Structures and Materials- Section 7 Stress Concentration
Structures and Materials- Section 7 Stress ConcentrationStructures and Materials- Section 7 Stress Concentration
Structures and Materials- Section 7 Stress Concentration
 
Presentation1
Presentation1Presentation1
Presentation1
 
IMPACT TEST REPORT ...
IMPACT TEST REPORT                                                           ...IMPACT TEST REPORT                                                           ...
IMPACT TEST REPORT ...
 
Compression test verification_for_a_wood
Compression test verification_for_a_woodCompression test verification_for_a_wood
Compression test verification_for_a_wood
 
Fracture Mechanics & Failure Analysis:Lecture Toughness and fracture toughness
Fracture Mechanics & Failure Analysis:Lecture Toughness and fracture toughnessFracture Mechanics & Failure Analysis:Lecture Toughness and fracture toughness
Fracture Mechanics & Failure Analysis:Lecture Toughness and fracture toughness
 
Vicker test
Vicker testVicker test
Vicker test
 
Rockwell hardnes testing
Rockwell hardnes testingRockwell hardnes testing
Rockwell hardnes testing
 
Fracture toughness measurement testing
Fracture toughness measurement testingFracture toughness measurement testing
Fracture toughness measurement testing
 
Hardness testing
Hardness testingHardness testing
Hardness testing
 
Fracture Toughness Lab
Fracture Toughness LabFracture Toughness Lab
Fracture Toughness Lab
 
Material testing
Material testingMaterial testing
Material testing
 
fracture mechanics presentation
fracture mechanics presentationfracture mechanics presentation
fracture mechanics presentation
 

Similaire à Nanoindentation mts meeting madrid 2007

Forming characterization and evaluation of hardness of nano carbon cast iron
Forming characterization and evaluation of hardness of  nano carbon cast ironForming characterization and evaluation of hardness of  nano carbon cast iron
Forming characterization and evaluation of hardness of nano carbon cast ironPadmanabhan Krishnan
 
The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...
The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...
The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...theijes
 
Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...
Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...
Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...IJERA Editor
 
IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...
IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...
IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...IRJET Journal
 
STUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETE
STUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETESTUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETE
STUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETEShoaib Wani
 
Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...
Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...
Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...IOSR Journals
 
MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...
MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...
MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...IAEME Publication
 
Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...
Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...
Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...IJERA Editor
 
STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...
STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...
STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...sivanagaraju chittelu
 
Vacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blanking
Vacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blankingVacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blanking
Vacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blankingEVP Vacuum pump
 
Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...
Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...
Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...IRJET Journal
 
SLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITES
SLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITESSLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITES
SLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITESIAEME Publication
 

Similaire à Nanoindentation mts meeting madrid 2007 (20)

Poster international tooling conference torino 2006
Poster international tooling conference torino 2006Poster international tooling conference torino 2006
Poster international tooling conference torino 2006
 
Forming characterization and evaluation of hardness of nano carbon cast iron
Forming characterization and evaluation of hardness of  nano carbon cast ironForming characterization and evaluation of hardness of  nano carbon cast iron
Forming characterization and evaluation of hardness of nano carbon cast iron
 
The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...
The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...
The Effects of Welding Processes and Microstructure on 3 Body Abrasive Wear R...
 
Ak26230233
Ak26230233Ak26230233
Ak26230233
 
Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...
Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...
Microstructural Characterization of Co-Cr-Mo-W Alloy as Casting for Odontolog...
 
IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...
IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...
IRJET- Experimental Analysis of Fracture Toughness and Microstructure Analysi...
 
DP-Triaxiality01.pdf
DP-Triaxiality01.pdfDP-Triaxiality01.pdf
DP-Triaxiality01.pdf
 
STUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETE
STUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETESTUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETE
STUDY ON BOND MECHANISM OF PSWC BARS WITH CONCRETE
 
A012130105
A012130105A012130105
A012130105
 
Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...
Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...
Effect of Notch Angle on the Fracture Toughness of Al7075 T6 Alloy- An Experi...
 
MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...
MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...
MICROSTRUCTURAL CHARACTERIZATION AND HOT EROSION BEHAVIOR OF CRC-NICR COATED ...
 
Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...
Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...
Mechanical Behaviour ofAl2014 Reinforced with Boron Carbide and Short Basalt ...
 
STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...
STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...
STRUCTURE PROPERTY CORRELATION OF MODIFIED Al-Mg ALLOYS FOR AEROSPACE APPLICA...
 
Vacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blanking
Vacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blankingVacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blanking
Vacuum furnace simuwu_improved_vacuum_heat-treatment_for_fine-blanking
 
D Day
D DayD Day
D Day
 
The effect of predeformation level on the variability of forming properties o...
The effect of predeformation level on the variability of forming properties o...The effect of predeformation level on the variability of forming properties o...
The effect of predeformation level on the variability of forming properties o...
 
W04408116121
W04408116121W04408116121
W04408116121
 
Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...
Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...
Corrosion Effects of Cr and Ni in Thermo-Mechanical Treated Steel Bar in Mari...
 
SLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITES
SLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITESSLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITES
SLIDING WEAR OF AA6061/CARBON BLACK METAL MATRIX COMPOSITES
 
Desouza2003
Desouza2003Desouza2003
Desouza2003
 

Plus de Fundació CTM Centre Tecnològic

Poster international conference on engineering failure analysis 2008
Poster international conference on engineering failure analysis 2008Poster international conference on engineering failure analysis 2008
Poster international conference on engineering failure analysis 2008Fundació CTM Centre Tecnològic
 
Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009
Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009
Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009Fundació CTM Centre Tecnològic
 
Study of transient stability for parallel connected inverters in microgrid sy...
Study of transient stability for parallel connected inverters in microgrid sy...Study of transient stability for parallel connected inverters in microgrid sy...
Study of transient stability for parallel connected inverters in microgrid sy...Fundació CTM Centre Tecnològic
 
Estudio de microgrids con interfases de convertidores de dc ac
Estudio de microgrids con interfases de convertidores de dc acEstudio de microgrids con interfases de convertidores de dc ac
Estudio de microgrids con interfases de convertidores de dc acFundació CTM Centre Tecnològic
 
Transient stability analysis of inverter interfaced distributed generators in...
Transient stability analysis of inverter interfaced distributed generators in...Transient stability analysis of inverter interfaced distributed generators in...
Transient stability analysis of inverter interfaced distributed generators in...Fundació CTM Centre Tecnològic
 
Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...
Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...
Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...Fundació CTM Centre Tecnològic
 
Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...
Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...
Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...Fundació CTM Centre Tecnològic
 

Plus de Fundació CTM Centre Tecnològic (20)

Conformabilitat v1
Conformabilitat v1Conformabilitat v1
Conformabilitat v1
 
Caracterizació ahss v2
Caracterizació ahss v2Caracterizació ahss v2
Caracterizació ahss v2
 
Effect of strain paths gutierrez et al
Effect of strain paths gutierrez et alEffect of strain paths gutierrez et al
Effect of strain paths gutierrez et al
 
Poster international conference on engineering failure analysis 2008
Poster international conference on engineering failure analysis 2008Poster international conference on engineering failure analysis 2008
Poster international conference on engineering failure analysis 2008
 
Poster congreso nacional de materiales donosti 2008
Poster congreso nacional de materiales donosti 2008Poster congreso nacional de materiales donosti 2008
Poster congreso nacional de materiales donosti 2008
 
Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009
Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009
Poster artdeco indo-ctm- microscratching of opthalmic coatings 2009
 
Poster congreso nacional de materiales vigo 2006
Poster congreso nacional de materiales vigo 2006Poster congreso nacional de materiales vigo 2006
Poster congreso nacional de materiales vigo 2006
 
Membrane capabilities ctm
Membrane capabilities ctmMembrane capabilities ctm
Membrane capabilities ctm
 
Poster grs 3040
Poster grs 3040Poster grs 3040
Poster grs 3040
 
Poster consoil 2010 respi
Poster consoil 2010 respiPoster consoil 2010 respi
Poster consoil 2010 respi
 
Poster consoil 2010 dh
Poster consoil 2010 dhPoster consoil 2010 dh
Poster consoil 2010 dh
 
Iwa 3018 poster
Iwa 3018 posterIwa 3018 poster
Iwa 3018 poster
 
Euromembrane 09 seawater
Euromembrane 09   seawaterEuromembrane 09   seawater
Euromembrane 09 seawater
 
Membrane technology summer school set_2011
Membrane technology summer school set_2011Membrane technology summer school set_2011
Membrane technology summer school set_2011
 
Euromembrane 09 trace ion method
Euromembrane 09   trace ion methodEuromembrane 09   trace ion method
Euromembrane 09 trace ion method
 
Study of transient stability for parallel connected inverters in microgrid sy...
Study of transient stability for parallel connected inverters in microgrid sy...Study of transient stability for parallel connected inverters in microgrid sy...
Study of transient stability for parallel connected inverters in microgrid sy...
 
Estudio de microgrids con interfases de convertidores de dc ac
Estudio de microgrids con interfases de convertidores de dc acEstudio de microgrids con interfases de convertidores de dc ac
Estudio de microgrids con interfases de convertidores de dc ac
 
Transient stability analysis of inverter interfaced distributed generators in...
Transient stability analysis of inverter interfaced distributed generators in...Transient stability analysis of inverter interfaced distributed generators in...
Transient stability analysis of inverter interfaced distributed generators in...
 
Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...
Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...
Effect of Burn-up and High Burn-up Structure on UO2 Spent Fuel Matrix Dissolu...
 
Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...
Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...
Ultrasound inspections on glass fiber/phenolicresin and on carbon fiber/epoxy...
 

Dernier

DBX First Quarter 2024 Investor Presentation
DBX First Quarter 2024 Investor PresentationDBX First Quarter 2024 Investor Presentation
DBX First Quarter 2024 Investor PresentationDropbox
 
Ransomware_Q4_2023. The report. [EN].pdf
Ransomware_Q4_2023. The report. [EN].pdfRansomware_Q4_2023. The report. [EN].pdf
Ransomware_Q4_2023. The report. [EN].pdfOverkill Security
 
Automating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps ScriptAutomating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps Scriptwesley chun
 
Exploring the Future Potential of AI-Enabled Smartphone Processors
Exploring the Future Potential of AI-Enabled Smartphone ProcessorsExploring the Future Potential of AI-Enabled Smartphone Processors
Exploring the Future Potential of AI-Enabled Smartphone Processorsdebabhi2
 
Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...
Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...
Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...apidays
 
Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...
Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...
Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...apidays
 
Real Time Object Detection Using Open CV
Real Time Object Detection Using Open CVReal Time Object Detection Using Open CV
Real Time Object Detection Using Open CVKhem
 
Cloud Frontiers: A Deep Dive into Serverless Spatial Data and FME
Cloud Frontiers:  A Deep Dive into Serverless Spatial Data and FMECloud Frontiers:  A Deep Dive into Serverless Spatial Data and FME
Cloud Frontiers: A Deep Dive into Serverless Spatial Data and FMESafe Software
 
Strategize a Smooth Tenant-to-tenant Migration and Copilot Takeoff
Strategize a Smooth Tenant-to-tenant Migration and Copilot TakeoffStrategize a Smooth Tenant-to-tenant Migration and Copilot Takeoff
Strategize a Smooth Tenant-to-tenant Migration and Copilot Takeoffsammart93
 
Corporate and higher education May webinar.pptx
Corporate and higher education May webinar.pptxCorporate and higher education May webinar.pptx
Corporate and higher education May webinar.pptxRustici Software
 
TrustArc Webinar - Stay Ahead of US State Data Privacy Law Developments
TrustArc Webinar - Stay Ahead of US State Data Privacy Law DevelopmentsTrustArc Webinar - Stay Ahead of US State Data Privacy Law Developments
TrustArc Webinar - Stay Ahead of US State Data Privacy Law DevelopmentsTrustArc
 
FWD Group - Insurer Innovation Award 2024
FWD Group - Insurer Innovation Award 2024FWD Group - Insurer Innovation Award 2024
FWD Group - Insurer Innovation Award 2024The Digital Insurer
 
Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...
Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...
Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...apidays
 
Navi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot Model
Navi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot ModelNavi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot Model
Navi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot ModelDeepika Singh
 
Polkadot JAM Slides - Token2049 - By Dr. Gavin Wood
Polkadot JAM Slides - Token2049 - By Dr. Gavin WoodPolkadot JAM Slides - Token2049 - By Dr. Gavin Wood
Polkadot JAM Slides - Token2049 - By Dr. Gavin WoodJuan lago vázquez
 
Manulife - Insurer Transformation Award 2024
Manulife - Insurer Transformation Award 2024Manulife - Insurer Transformation Award 2024
Manulife - Insurer Transformation Award 2024The Digital Insurer
 
ICT role in 21st century education and its challenges
ICT role in 21st century education and its challengesICT role in 21st century education and its challenges
ICT role in 21st century education and its challengesrafiqahmad00786416
 
How to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected WorkerHow to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected WorkerThousandEyes
 
Strategies for Landing an Oracle DBA Job as a Fresher
Strategies for Landing an Oracle DBA Job as a FresherStrategies for Landing an Oracle DBA Job as a Fresher
Strategies for Landing an Oracle DBA Job as a FresherRemote DBA Services
 

Dernier (20)

DBX First Quarter 2024 Investor Presentation
DBX First Quarter 2024 Investor PresentationDBX First Quarter 2024 Investor Presentation
DBX First Quarter 2024 Investor Presentation
 
Ransomware_Q4_2023. The report. [EN].pdf
Ransomware_Q4_2023. The report. [EN].pdfRansomware_Q4_2023. The report. [EN].pdf
Ransomware_Q4_2023. The report. [EN].pdf
 
Automating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps ScriptAutomating Google Workspace (GWS) & more with Apps Script
Automating Google Workspace (GWS) & more with Apps Script
 
Exploring the Future Potential of AI-Enabled Smartphone Processors
Exploring the Future Potential of AI-Enabled Smartphone ProcessorsExploring the Future Potential of AI-Enabled Smartphone Processors
Exploring the Future Potential of AI-Enabled Smartphone Processors
 
Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...
Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...
Apidays New York 2024 - The Good, the Bad and the Governed by David O'Neill, ...
 
Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...
Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...
Apidays New York 2024 - Accelerating FinTech Innovation by Vasa Krishnan, Fin...
 
Real Time Object Detection Using Open CV
Real Time Object Detection Using Open CVReal Time Object Detection Using Open CV
Real Time Object Detection Using Open CV
 
Cloud Frontiers: A Deep Dive into Serverless Spatial Data and FME
Cloud Frontiers:  A Deep Dive into Serverless Spatial Data and FMECloud Frontiers:  A Deep Dive into Serverless Spatial Data and FME
Cloud Frontiers: A Deep Dive into Serverless Spatial Data and FME
 
Strategize a Smooth Tenant-to-tenant Migration and Copilot Takeoff
Strategize a Smooth Tenant-to-tenant Migration and Copilot TakeoffStrategize a Smooth Tenant-to-tenant Migration and Copilot Takeoff
Strategize a Smooth Tenant-to-tenant Migration and Copilot Takeoff
 
Corporate and higher education May webinar.pptx
Corporate and higher education May webinar.pptxCorporate and higher education May webinar.pptx
Corporate and higher education May webinar.pptx
 
+971581248768>> SAFE AND ORIGINAL ABORTION PILLS FOR SALE IN DUBAI AND ABUDHA...
+971581248768>> SAFE AND ORIGINAL ABORTION PILLS FOR SALE IN DUBAI AND ABUDHA...+971581248768>> SAFE AND ORIGINAL ABORTION PILLS FOR SALE IN DUBAI AND ABUDHA...
+971581248768>> SAFE AND ORIGINAL ABORTION PILLS FOR SALE IN DUBAI AND ABUDHA...
 
TrustArc Webinar - Stay Ahead of US State Data Privacy Law Developments
TrustArc Webinar - Stay Ahead of US State Data Privacy Law DevelopmentsTrustArc Webinar - Stay Ahead of US State Data Privacy Law Developments
TrustArc Webinar - Stay Ahead of US State Data Privacy Law Developments
 
FWD Group - Insurer Innovation Award 2024
FWD Group - Insurer Innovation Award 2024FWD Group - Insurer Innovation Award 2024
FWD Group - Insurer Innovation Award 2024
 
Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...
Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...
Apidays Singapore 2024 - Building Digital Trust in a Digital Economy by Veron...
 
Navi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot Model
Navi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot ModelNavi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot Model
Navi Mumbai Call Girls 🥰 8617370543 Service Offer VIP Hot Model
 
Polkadot JAM Slides - Token2049 - By Dr. Gavin Wood
Polkadot JAM Slides - Token2049 - By Dr. Gavin WoodPolkadot JAM Slides - Token2049 - By Dr. Gavin Wood
Polkadot JAM Slides - Token2049 - By Dr. Gavin Wood
 
Manulife - Insurer Transformation Award 2024
Manulife - Insurer Transformation Award 2024Manulife - Insurer Transformation Award 2024
Manulife - Insurer Transformation Award 2024
 
ICT role in 21st century education and its challenges
ICT role in 21st century education and its challengesICT role in 21st century education and its challenges
ICT role in 21st century education and its challenges
 
How to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected WorkerHow to Troubleshoot Apps for the Modern Connected Worker
How to Troubleshoot Apps for the Modern Connected Worker
 
Strategies for Landing an Oracle DBA Job as a Fresher
Strategies for Landing an Oracle DBA Job as a FresherStrategies for Landing an Oracle DBA Job as a Fresher
Strategies for Landing an Oracle DBA Job as a Fresher
 

Nanoindentation mts meeting madrid 2007

  • 1. Fracture toughness of carbides in tool steels evaluated by nanoindentation J. Caro a , D. Casellas a , S. Molas a , J. M. Prado a , I. Valls b a CTM Centre Tecnològic b ROVALMA S.A.
  • 2.
  • 3.
  • 4.
  • 5. INTRODUCTION In order to develop high performance tool steels is necessary a detailed knowledge of the relationship between the hardness and fracture toughness of carbides and the macroscopic wear and fracture resistance of the bulk material The micrometric size of primary carbides to be analyzed forces the use of nanoindentation techniques Hardness and Young modulus : determined by confined indentation on carbides Fracture toughness : determined by the generation of cracks at the corner of the indentation This work has been recently published in D. Casellas et al., Acta Materialia 55 (2007) 4277 INTRODUCTION
  • 6. In brittle materials fracture toughness (K C ) can be determined by the Indentation Microfracture Method (IM) Types of fracture generated by sharp indenters Halfpenny or radial cracks Connected underneath the hardness impression. The most common crack configuration for brittle materials Palmqvist cracks Developed at low indentation loads or in high-toughness materials (i.e. hard metals or zirconia ceramics) Berkovich cracks FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 7. Common expression used for K C determination (depending on indenter geometry and crack morphology): Anstis. : Limited to radial cracks. Applied to the symmetric indenters (i.e. Vickers) P indentation load, c crack length A = 0.016 and n =0.5 Laugier : Used for Palmqvist cracks x V = 0.015 Niihara : Used for Palmqvist cracks a : half-diagonal of the impression c = a + l  = 0.0089 (for WC-Co) [1] [2] [3] FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 8. FRACTURE TOUGHNESS FRACTURE TOUGHNESS Berkovich indenters are generally used in small-scale determination of K C . The most commonly used expression is Anstis equation. However, the nonsymmetrical nature of Berkovich indenters does not permit the radial cracks to be joined beneath the hardness impression The application of Anstis equation in this case is doubtful Dukino and Swain determined that good K c values using Berkovich indenters are obtained using Laugier expression with a little modification (x V = 0.016)
  • 9. In this work, K C of micrometric primary carbides (10-20  m) in tool steels is determined using Berkovich indenters at low indentation loads (200-500 mN). It is expected to generate Palmqvist-type cracks (equations 2-3 are expected to give better results than equation 1). It is necessary to generate small cracks (shorten than 5-10  m) within the carbide. At this crack extension application of equations (1)-(3) could give rise to considerable differences in the calculated K C value. FRACTURE TOUGHNESS FRACTURE TOUGHNESS 9  m
  • 10. Values of K C evaluated with expressions (1)-(3) for different primary carbides in different tool steels FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 11. K C values calculated by the expressions (1)-(3) at P=200 mN and a=2.8  m corresponding to the M 6 C carbides of 1.3202 steel. At short crack lengths Laugier’s expression (3) gives the highest values of K C , 2.4 times larger than Anstis’s expression (1) FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 12. As postulated previously, Laugier’s expression seems to be more appropriate for nanoindentation tests using Berkovich indenters. This expression has been successfully proved in a wide range of ceramic materials using Berkovich indenters. However, the differences between the results obtained with different expressions should be assessed. Consequently, the IM method was applied to a material whose K C is well known using low loads. The results were compared with the K C values obtained with macroscopic methods based on the propagation and fracture of large cracks reported in the literature. Chosen material  Silicon single crystal Si (100) FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 13. Nanoindentation on Si(100) plane at 200 mN Niihara (2) and Laugier (3) (using x V = 0.016) expressions give values of K C within the range of the values of Si reported with large crack testing methods FRACTURE TOUGHNESS FRACTURE TOUGHNESS large crack testing methods
  • 14. Niihara et al. set the applicability of equation (2) within the range 0.4<a/l<1 In our case, almost all the data for the analyzed carbides lie outside this range FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 15. CONCLUSION: All these comments allow us to point out that the evaluation of K C by nanoindentation using Berkovich indenters should be conducted using Laugier expression (with x V = 0.016): This assertion is specially relevant at low applied loads, when cracks are shorten than 10  m, which usually occurs in nanoindentation of small particles such as in primary carbides of commercial cold work tool steels FRACTURE TOUGHNESS FRACTURE TOUGHNESS
  • 16.
  • 17. RESULTS RESULTS Crystal structure was determined by XRD Samples were extracted with the same orientation, parallel to the rolling direction
  • 18.
  • 19. RESULTS RESULTS catastrophic carbide fracture 20  m 20  m catastrophic carbide fracture
  • 20.
  • 21. RESULTS RESULTS 1.3202 Steel M 6 C M 6 C MC 7  m 10  m 10  m
  • 22. RESULTS RESULTS MC-II Steel B 15  m MC-I Steel A 9  m 8  m MC-III Steel B
  • 23. RESULTS Fracture anisotropy in M 7 C 3 carbides in 1.2379
  • 24.
  • 25. RESULTS RESULTS Arrows for M 7 C 3 in 1.2379 steel indicate that K C may be even lower Hardness and fracture toughness of different carbides Hard and tough carbides Potential candidates for incorporating in tool steels aimed at optimizing the relationship between wear and fracture resistance
  • 26. RESULTS RESULTS Toughness (K C ) vs. composition of MC carbides V-rich carbides exhibit high values of K C